Guides › How to fix stringing in 3D prints
How to fix stringing in 3D prints
Short answer: dry the filament, lower the nozzle temperature 5–10 °C, then tune retraction (about 0.5–1 mm on a direct-drive extruder, 4–6 mm on a Bowden). Most stringing is caused by one of those three things, in that order.
What stringing actually is
When the nozzle travels across open space, molten plastic in the nozzle keeps oozing out under its own pressure and gravity. The thin trail it leaves cools into “hairs” between parts. Retraction pulls the filament back to relieve that pressure before the travel, and lower temperatures make the plastic thicker so it oozes less. Moisture makes it worse because water turns to steam in the nozzle and pushes extra plastic out.
Fix it in this order
- Dry the filament. Wet PETG, TPU and nylon string no matter how good the retraction is. Popping or hissing at the nozzle confirms it. See the drying chart.
- Print a temperature tower. Pick the coolest section that still has strong layers. Our temperature tower generator adds the changes to any G-code.
- Tune retraction distance. Change 0.2 mm at a time on direct drive or 0.5 mm on Bowden.
- Tune retraction speed. 25–45 mm/s is typical. Too fast can grind filament.
- Adjust travel. Raise travel speed, enable “combing” or “avoid crossing perimeters” so the nozzle travels over the part instead of open air.
Starting retraction values
| Setup | Distance | Speed |
|---|---|---|
| Direct drive, PLA | 0.5–1.0 mm | 30–45 mm/s |
| Direct drive, PETG | 0.8–1.5 mm | 25–40 mm/s |
| Bowden, PLA | 4–6 mm | 40–50 mm/s |
| Bowden, PETG | 5–7 mm | 30–45 mm/s |
| TPU, direct drive | 0–1 mm | 20–30 mm/s |
Typical starting ranges; your hotend and extruder will differ. Pressure advance or linear advance, once calibrated, often lets you reduce retraction further (see the pressure advance calculator). For a starting distance and speed for your exact setup, use the retraction calculator.
Worked example
A PETG print on a direct-drive printer strings badly at 245 °C with 0.8 mm retraction. Step 1: the spool pops at the nozzle, so it goes in the dryer for 6 hours at 65 °C. Stringing drops by about half. Step 2: a temperature tower from 250 to 220 °C shows that 235 °C still bonds well. Step 3: retraction goes from 0.8 to 1.2 mm in two steps. The remaining wisps are removed in seconds with a heat gun on low. Total changes: three settings, no new hardware.
Common mistakes
- Cranking retraction to 10 mm on direct drive. This pulls molten plastic into the cold zone and causes clogs.
- Changing several settings at once. You will not know which one worked.
- Ignoring moisture. No setting fixes wet filament.
- Blaming retraction for “blobs and zits”. Those come from seams and pressure; try seam placement and pressure advance.
Troubleshooting
| Symptom | Likely cause | Fix |
|---|---|---|
| Fine hairs everywhere | Too hot or wet | Dry, then lower temperature |
| Thick strings | Too little retraction | Increase in small steps |
| Gaps after travel | Too much retraction, or ooze before travel | Reduce retraction, add a small extra prime |
| Clicking extruder after tuning | Retraction too fast or long | Slow it to 30 mm/s |
Keep reading
- How to fix layer shifting
- Heat-set insert hole sizes
- Filament temperature chart
- How to fix under-extrusion
- How to fix elephant's foot
Recommended gear
- Filament dryer — Dries while you print. Check max temperature (≥70 °C) if you print nylon.
- Overture High Speed PETG, 1 kg — Tougher and more heat-resistant than PLA for functional parts.
- Overture High Speed PLA, 1 kg (1.75 mm) — Our default PLA pick: tight ±0.02 mm diameter tolerance and fast-print friendly.
Some links are affiliate links. MeshMath earns a commission on purchases made through Overture and Anycubic (via Awin) links, at no extra cost to you. Picks are chosen for usefulness, not paid placement.
Tools for this
E-steps & flow calibration calculator
Calibrate extruder e-steps and flow rate, with the exact M92 G-code to send.
Temperature tower G-code generator
Add temperature changes by height to any sliced G-code file.
Filament drying temperature & time chart
How hot and how long to dry PLA, PETG, TPU, Nylon and more.
Retraction distance & speed calculator
Starting retraction distance, speed and Z-hop for direct drive or Bowden, by material and nozzle.