Short answer: warping happens because plastic shrinks as it cools, and the top of the part shrinks while the bottom is held to the bed. Keep the part warm and evenly cooled (enclosure for ABS/ASA, no draughts for anything), make the first layer stick well, and add a brim. Design changes like rounded corners help more than people expect.
Why it happens
Every plastic contracts as it cools from printing temperature to room temperature. ABS shrinks noticeably more than PLA, which is why ABS warps so readily. Each new layer is laid down hot and pulls on the cooler layers beneath it. If the pull is stronger than the bond to the bed, corners lift. Long, flat, sharp-cornered parts suffer most because the stress concentrates at the corners.
Settings by material
| Material | Bed | Part fan | Enclosure | Warp risk |
|---|---|---|---|---|
| PLA | 55–65 °C | 100% | No (can cause heat creep) | Low |
| PETG | 70–85 °C | 30–50% | Optional | Low–medium |
| ABS | 100–110 °C | 0–20% | Yes | High |
| ASA | 95–110 °C | 0–30% | Yes | High |
| Nylon | 70–90 °C | 0–30% | Yes | High |
Fixes, most effective first
- Stop draughts. A window, air conditioner or ceiling fan can warp even PLA. An enclosure or a cardboard box over the printer helps.
- Improve first-layer grip. See first layer adhesion.
- Add a brim of 5–10 mm, or “mouse ears” (small discs) at sharp corners.
- Reduce cooling for ABS, ASA and nylon.
- Change the design: round corners with a 3–5 mm fillet, split long parts, or add slots that relieve stress.
- Choose a less warp-prone material: ASA warps less than ABS for outdoor parts; PETG is a good middle ground.
Worked example
A 200 × 30 × 15 mm ABS rail lifts 2 mm at both ends in an open printer. Adding a cardboard enclosure raises the air temperature around the part from 22 °C to about 40 °C and halves the lift. Adding an 8 mm brim and 4 mm fillets on the corners in CAD removes the remaining warp. The part fan, which had been at 30%, is turned off.
Common mistakes
- Raising the bed temperature for PLA to 80 °C. This softens the lower layers and causes elephant’s foot instead.
- Opening the enclosure door mid-print to check progress.
- Removing ABS parts while the bed is hot can bend them; let them cool.
Troubleshooting
| Symptom | Fix |
|---|---|
| Corners lift in the first few layers | Adhesion: clean bed, Z offset, brim |
| Part lifts after 10–20 mm | Shrinkage stress: enclosure, less fan |
| Cracks between layers (ABS) | Chamber too cold; enclose and stop draughts |
| Only one side warps | Draught from one side, or uneven bed heat |
Keep reading
- How to fix layer shifting
- Heat-set insert hole sizes
- Filament temperature chart
- How to fix under-extrusion
- How to fix elephant's foot
Recommended gear
- Textured PEI build plate — Reliable adhesion and easy release; check your printer’s size.
- Overture High Speed PETG, 1 kg — Tougher and more heat-resistant than PLA for functional parts.
- Filament dryer — Dries while you print. Check max temperature (≥70 °C) if you print nylon.
Some links are affiliate links. MeshMath earns a commission on purchases made through Overture and Anycubic (via Awin) links, at no extra cost to you. Picks are chosen for usefulness, not paid placement.
Tools for this
Temperature tower G-code generator
Add temperature changes by height to any sliced G-code file.
3D print tolerance & hole size calculator
Hole and peg sizes for press, snug, sliding and loose fits, M2–M10 bolts.
Filament drying temperature & time chart
How hot and how long to dry PLA, PETG, TPU, Nylon and more.